Warning: fopen(/home/virtual/kwjs/journal/upload/ip_log/ip_log_2024-05.txt): failed to open stream: Permission denied in /home/virtual/lib/view_data.php on line 88 Warning: fwrite() expects parameter 1 to be resource, boolean given in /home/virtual/lib/view_data.php on line 89 Microstructure and Hardness of Surface Melting Hardened Zone of Mold Steel, SM45C using Yb:YAG Disk Laser

Microstructure and Hardness of Surface Melting Hardened Zone of Mold Steel, SM45C using Yb:YAG Disk Laser

Article information

J Weld Join. 2016;34(1):75-81
* Korea Institute of Machinery & Materials, Busan Laser Application Support Center, Busan 46747, Korea
** Dept. of Material Science and Engineering, Pusan National University, Busan 46239, Korea
*** National core research center, Pusan National University, Busan 46239, Korea
Corresponding author : kangcy@pusan.ac.kr
Received 2016 February 3; Revised 2016 February 15; Accepted 2016 February 18.

Abstract

This study applied laser surface melting process using CW(Continuous wave) Yb:YAG laser and cold-work die steel SM45C and investigated microstructure and hardness. Laser beam speed, power and beam interval are fixed at 70 mm/sec, 2.8 kW and 800 μm respectively. Depth of Hardening layer(Melting zone) was a minimum of 0.8 mm and a maximum of 1.0 mm that exceeds the limit of minimum depth 0.5 mm applying trimming die. In all weld zone, macrostructure was dendrite structure. At the dendrite boundary, Mn, Al, S and O was segregated and MnS and Al oxide existed. However, this inclusion didn’t observe in the heat-affected zone (HAZ). As a result of interpreting phase transformation of binary diagram, MnS crystallizes from liquid. Also, it estimated that Al oxide forms by reacting with oxygen in the atmosphere. The hardness of the melting zone was from 650 Hv to 660 Hv regardless of the location that higher 60 Hv than the hardness of the HAZ that had maximum 600 Hv. In comparison with the size of microstructure using electron backscatter diffraction(EBSD), the size of micro-structure in the melting zone was smaller than HAZ. Because it estimated that cooling rate of laser surface melting process is faster than water quenching.

1. Introduction

SM45C, medium carbon steel, is widely used in industrial field for the production of machine parts such as crank and gear as well as the material of cold-work die steel. However, there can be damage such as abrasion easily when it is used for forming or cutting of advanced high strength steels which is currently increasing in use though it is used after surface hardening process on the material through surface preparation such as heat treatment1,2). To improve this problem, surface modification such as chemical vapor deposition (CVD), physical vapor deposition (PVD) has been applied3-5), however, the separation phenomenon has been frequently reported due to thin hardened layer depth and brittleness6).

This problem can be improved by increasing the hardened layer depth and combine the base material and hardened layer closely7). Laser surface melting hardening technology is a surface modification technology of material using rapid heating and cooling feature of laser. Especially, laser is proper for surface hardening of mold material because the hardened layer can be formed deeply, no limitation in material shape, and selective laser surface treatment is possible on the part need to be hardened. Based on these technical features, several researches for laser surface melting hardening have been reported currently8-10). However, Shin et al., reported that the hardened layer is about 300 μm in surface hardening using Nd:YAG laser11). Choi et al., reported that enough hardened layer depth (400∼500 μm) cannot be assured when hardening by diode laser7).

It is reported that Mo, Cr, V, and C which are included in the steel can form precipitation and attain grain refining by heat treatment. Additionally strength, hardness, abrasion resistance, and corrosion resistance are improved by forming microstructure such as martensite which is high in hardness by laser surface hardness1). However, in case of SM45C, it is difficult to expect the surface hardening by carbide forming because there is few carbide forming elements in it. Alain Kusmoko et al,. reported that the reason of hardening heat treatment of SM45C is the phase transformation of martensite12). Especially, in case of melting hardening using laser heat source, researchers reported that the mechanical property and hardened layer depth are different with the microstructure of hardened layer formed by existing heat treatment process due to the repetition of extreme rapid heating and cooling13). Although the SM45C of die steel is used in many cases, the study on the mechanism for laser surface melting hardening is nothing at all. Therefore, in this research, systematically study the correlation between the change in microstructure of surface melted part and heat-affected zone and hardness on the SM45C, medium carbon steel, on laser surface melting hardening process with minimum over 600 μm hardness depth using Yb:YAG high power disc laser.

2. Experimental Procedures

The chemical composition of SM45C steel used in this research is shown in Table 1, and the specimen thickness is 15mm. The surfaces of the specimen were mechanically worked as even and flat. The laser used for laser melting hardening treatment was Yb:YAG disc laser and the maximum output is 8 kW (Trumpf Tru Disk8002, Busan Laser Technology Support Center, Korea Institute of Machinery & Materials). The optical system of 0.4 mm beam diameter was used and being installed on 6-axes laser precision processing robot. Laser melting hardening treatment condition are fixed as laser focusing size of 400 μm, laser processing speed of 70 mm/s, beam interval of 800μm, and laser power of 2.8 kW. Ar gas (8 L/min) was supplied as shielding gas and the laser surface melting hardening treatment was performed as zigzag direction as shown in Fig. 1(a).

Chemical composition of SM45C

Fig. 1

Schematic illustration of laser hardening (a), Experimental equipment of laser surface melted hardening (b)

The microstructure of hardened layer was observed with optical microscope and scanning electron microscope(SEM) by revealing the structure using viela solution {CH3OH (100 mL) + HCl (4 mL) + Picric (1 g)} after grind the specimen. To analyze composition profile in melted zone, field emission electron probe micro analyzer (FE-EPMA) zone analysis was used and EBSD was used in comparison of melted zone and heat-affected zone grain size. To investigate the phase transformation on each zone, Thermo - Calc.™ (TCW) was used. The hardness of melted zone, heat-affected zone and the base material was measured using micro vickers hardness with 300 kgf load and time duration 10 seconds.

3. Result and Discussion

3.1 Hardness Distribution and Micro Structure of Surface Melted Hardened Zone

Fig. 2 is surface melted bead, and left side is finally formed bead. Average bead maximum depth of penetration is 1.0 mm and minimum is 0.8 mm, and the width of bead is 1.1mm.

Fig. 2

Cross-section of laser surface melting layer

Surface melted hardened layer is formed by bead overlapped with 0.8mm distance, so preceding bead is partially remelted by following laser beam, and forms heat-affected zone by the heat effect. Meted zone can be divided as melted zone (MZ) formed by following laser beam, remelted zone (RMZ) formed by remelting of MZ by preceding laser beam, heat affected zone in MZ (HAZMZ) formed by heat effect, and heat affected zone in base metal (HAZBM) formed on base material as shown in Fig. 3. Each zone has different forming procedure, so the hardness of each zone expected as different, therefore, vickers hardness were laterally measured with 100 μm distance, and also measured with 100 μm distance to depth direction to include MZ, RMZ, and HAZ at 100 μm under the surface as shown in Fig. 3. Fig. 4 shows the hardness distribution of each lateral (a) and depth direction (b). The lateral hardness distribution shows about ±4 hardness value deviation according to the location, and it means there is almost no difference. Also, the hardness value difference for depth direction according to the location in MZ has less difference; however, it is rapidly decreased from HAZ to BM.

Fig. 3

Schematic illustration of lase surface melting layer

Fig. 4

Hardness distributions of width(a) and depth(b) direction in the melting zone

Microstructure in MZ, RMZ, and HAZMZ in melted zone were compared to understand the reason of almost same hardness value for each area in MZ and the results were shown in Fig. 5. Fig. 5(a), (b), and (c) shows the microstructure observed by optical microscope for each MZ, RMZ, and HAZMZ, and Fig. 5(d), (e), and (f) shows the magnified microstructure marked as ☐ for (a), (b), and (c) by SEM. Fig. 6 is the solidification microstructure in MZ observed by OM. Based on the comparison between Fig. 5 and Fig. 6, black band type part in Fig. 5 can be identified as dendrite boundary. In the microstructure from OM and SEM in Fig. 5, the difference according to the zone in MZ.

Fig. 5

Optical microstructures and SEM structures of laser surface melting layer (a), (d) melted zone, (b),(e) remelted zone, (c), (f) HAZ in previous melted zone

Fig. 6

Optical microstructures of laser surface melted zone

Fig. 7(a) and (b) shows the microstructure in MZ by OM and SEM, and Fig. 7(c) to (h) reveals the result of elemental mapping analysis by EPMA corresponding Fig. 7(b). Based on it, it is indicated that the band zone in microstructure segregates Mn and Si, and concentrated Al, S, and O shaped spheral type are existed in it. That is, MnS and Al based oxide are existed in it.

Fig. 7

Optical(a), SEM(b) microstructure and EPMA mapping results showing distribution of elements in melted zone

Fig. 8 shows the microstructure of BM by SEM, and it shows that BM has layer structure with ferrite and pearlite and no inclusion is existed.

Fig. 8

SEM microstructure of the base metal

Therefore, the segregation layer formed on surface MZ and the band zone with MnS, Al based oxide were expected forming during the solidification after melting.

3.2 Hardness and .micro structure between melted zone and base material

Fig. 9 shows the macrostructure between MZ and BM observed by OM. By this macrostructure, the microstructure cannot be classified, so the BM/HAZ interface part and HAZ/MZ interface part were magnified as indicated as A and B in the figure. Fig. 10(a) is the magnified microstructure of BM/HAZ interface part by SEM, and Fig. 10(b) to (e) are the magnified microstructure of BM, H1-H3 indicated in Fig. 10(a) by SEM. The proeutectoid ferrite (F) is decreased from BM to MZ in Fig. 10(a). Also, by the comparison of Fig. 10(b) to (e), from BM (b) to H3 (e), the lamella structure in pearlite gradually disappears and changes to new needlelike structure, therefore, ferrite is not exist and almost needlelike structure at H4 (e). Fig. 11(a) is magnified microstructure of HAZ/MZ (B) interface part by SEM, and Fig. 11(b) to (e) are magnified microstructure of H4-M2 indicated in (a) by SEM. Based on the comparison between Fig. 10(a) and Fig. 11(a), ferrite is almost not shown, and lamella structure perlite is not observed. In the comparison of HAZ ((b), (c)) and MZ (d), there are MnS and Al based oxide in MZ, but not existed in HAZ. Based on it, it is identified that inclusions are formed during the solidification. Table 2 shows BM to M2 in Fig. 10.

Fig. 9

Optical microstructure between the melted zone and the base metal

Fig. 10

(a)SEM structures from the base metal to HAZ, (b)-(e) enlarged SEM structures of area denoted as BM, H1, H2, H3 in (a)

Fig. 11

(a)SEM structures from HAZ to melted zone, (b)-(e) enlarged SEM structures of area denoted as H4, H5, M1, M2 in (a)

Hardness near area denoted as x in (a) Fig. 10 and Fig. 11

The needlelike structure in HAZ and MZ is martensite, and it seems that the reason of increasing hardness from BM to MZ is that the ferrite is disappeared and pearlite transformed to martensite.

Especially, HAZ (melted zone boundary) and MZ is consisted with martensite completely, but the hardness in MZ is higher over about 60 Hv. It is expected by the difference of martensite, so compared the martensite size using EBSD. Fig. 12 is the analyzed result of H5 and M1 zone using EBSD in Fig. 11.

Fig. 12

Results obtained by EBSD. (a),(b) image quality map, (c), (d) inverse pole figure map. (a), (c) HAZ, (b), (d) MZ

Fig. 11(a) and (b) is image quality (IQ) map showing crystal grain classified with average mean strength by Kikuchi band, and Fig. 11(c) and (d) is inverse pole figure (IPF) map divided with color for crystal orientation of crystal grain. Fig. 11(a) and (c) have been resulted from H5, and Fig. 11(b) and (d) are from M1. From this, the hardness in fusion zone (FZ) is higher than that of HAZ because martensite size of FZ is much refined. However, the austenite in FZ is more refiner because the austenite in HAZ is created and grown by reheating. On the other hand, austenite in FZ is formed during the solidification by rapid cooling. Therefore, the cooling speed is same, so it is considered that the martensite size is refined because the austenite in FZ is refined.

3.3 Phase transformation of surface melted hardened zone

To understand the phase transformation process of MZ inside and BM/HAZ boundary during the melting and cooling process by laser beam, binary system constitutional diagram is prepared using Thermo-Calc.™ (TCW5) software.

Fig. 13 is binary system constitutional diagram of Fe (0.70 Mn- 0.28 Si- 0.02 Cr- 0.04 Al- 0.05 S) - C, and the figures for the marked zone numbers were expressed on the constitutional diagram. The formation of dendrite cores occurs because the almost austenite (γ) formed by faster cooling speed during solidification of liquid phase of BM (0.41 wt%C). As the solidification is processed, Mn, Si, and Al are segregated, and MnS is crystallized on dendrite boundary at end of solidification (about 1,400 °C) and finishing the solidification. And the segregated Mn and Al based oxide by the reaction with oxygen in the air.

Fig. 13

Quasi-binary phase diagram for calculated using Thermo-Calc™ software

Generally, the cooling speed of laser beam welding is 605 °C/s, and it is known that the cooling speed is faster than water cooling15). So, the austenite (γ, middle of dendrite) transforms as martensite due to the rapid cooling.

Meanwhile, the phase transformation of HAZ (HAZBM) in the BM is as follows. It is heated as 6 zone (A1-A3 temperature) in phase diagram; solution of cementite occurred in perlite, so transformed as γ, and increasing γ volume by decreasing and disappearance of ferrite when the temperature is increased. At the 5 zone temperature range, completely transformed as γ, and transforms to martensite due to the rapid cooling.

Generally, the heating by laser beam is rapid heating, so the phase transformation will be shown on higher temperature than indicated in the constitutional diagram.

4. Conclusion

Based on the review on microstructure and hardness features of SM45C treated as surface melting hardening with Yb:YAG disc laser, the experiment result is as follows.

  • 1) The depth of surface melting hardening layer was minimum 0.8mm, maximum 1.0mm.

  • 2) The hardness of surface melted zone inside was 650-660 Hv without reference to the location, and it is about 60 Hv higher than HAZ maximum hardness (590-600 Hv). Based on the comparison of micro structure between melted zone and HAZ by EBSD, the hardness of melted zone is higher because the microstructure is minute.

  • 3) The cooling speed of laser surface melting hardening treatment is 605 °C/s (calculated with t85 formula) and it is faster than water cooling, so the melted zone transformed as complete martensite, and the microstructure is very minute.

  • 4) The macrostructure inside surface melted zone has dendrite form; also there are Mn, Si element segregate at the dendrite boundary, MnS at dendrite boundary, and Al based oxide in transgranular. However, there are no such inclusions in HAZ. Based on the interpretation of phase transformation with binary system constitutional diagram, Mns was crystallized in liquid state, and Al affiliation oxide was seems to be formed with oxygen in the air. Segregated Mn and Si, and concentrated sphere shaped Al, S, and O is existed at the band zone in the microstructure.

Acknowledgement

This work was supported by a 2-Year Research Grant of Pusan National University

References

1. Telasang G, Majumdar JD, Padmanabham G, Manna I. Structure-property correlation in laser surface treated AISI H13 tool steel for improved mechanical properties. Materials Science Engineering A 5992014;:255–267.
2. Zhang Z, Lin P, Cong D, Kong S, Zhou H, Ren L. The characteristics of treated zone processed by pulsed Nd-YAG laser surface remelting on hot work steel. Optics & Laser Technology 642014;:227–234.
3. Wang C, Zhou H, Liang N, Wang C, Cong D, Meng C, Ren L. Mechanical properties of several laser remelting processed steels with different unit spacings. Applied Surface Science 3132014;:333–340.
4. Kwok C.T, Cheng F.T, Man H.C. Microstructure and corrosion behavior of laser surface-melted high-speed steels. Surface & Coatings Technology 2022007;:336–348.
5. Yasavola N, Abdollah-zadeh A, Ganjali M, Alidokht SA. Microstructure and mechanical behavior of pulsed laser surface melted AISI D2 cold work tool steel. Applied Surface Science 2652013;:653–662.
6. Telasang G, Dutta Majumdar J, Padmanabham G, Manna I. Wear and corrosion behavior of laser surface engineered AISI H13 hot working tool steel. Surface and Coatings Technology 2612015;:69–78.
7. Choi Hong-Seok, Kim Byung-Min, Ko Dae-Cheol. Effect of clearance and inclined angle on sheared edge and tool failure in trimming of DP980 sheet. Journal of Mechanical Science and Technology 28(6)2014;:2319–2328.
8. Dutta Majumdar J, Galun R, Mordike B.L, Manna I. Effect of laser surface melting on corrosion and wear resistance of a commercial magnesium alloy. Materials Science and Engineering A 3612003;:119–129.
9. Oh Sae-Kyoo, Park Il-Dong, Jeon Tae-Eun, Lee Won-Suk. Friction Welding of Dissimilar Press Punch Materials and Its Evaluation By AE. Journal of KWJS 151997;:43–53. (in Korean).
10. Grum J, Sturm R. Influence of laser surface melthardening conditions on residual stresses in thin plates. Surface and Coatings Technology 100-1011998;:455–458.
11. Shin H.J, Yoo Y.T, Ahn D.G, Im K. Laser surface hardening of S45C medium carbon steel using Nd:YAG laser with a continuous wave. Journal of Materials Processing Technology 187-1882007;:467–470.
12. Kusmoko A, Dahar R, Li H. J, Hadi S. A Study Surface Layer and Hardness Produced by Induction Hardened S45C Steel. Applied Mechanics and Materials 6642014;:43–47.
13. Lee Kwang-Hyeon, Choi Seong-Won, Yun Jung Gil, Oh Myeong-Hwan, Kim Byung Min, Kang Chung-Yun. Effects of laser power on hardness and microstructureof the surface melting hardened SKD61 hotdie steel using Yb:YAG disk laser. Journal of KWJS 33-32015;:54–61. (in Korean).
14. Lee Kwang-Hyeon, Choi Seong-Won, Yun Jung Gil, Oh Myeong-Hwan, Kim Byung Min, Kang Chung-Yun. Microstructure and Hardness of Yb:YAG Disc Laser Surface Overlap Melted Cold Die Steel, STD11. Journal of KWJS 33-52015;:53–60. (in Korean).
15. Bonek M, Dobrzański LA, Hajduczek E, Klimpel A. Structure and properties of laser alloyed surface layers on the hot-work tool steel. Journal of Materials Processing Technology 1752006;:45–54.

Article information Continued

Table 1

Chemical composition of SM45C

SM45C Chemical composition (wt.%)
C Mn Si Cr Ni Mo V W P S Fe
0.41 0.70 0.25 0.02 0.03 - - - 0.03 0.05 Bal.

Fig. 1

Schematic illustration of laser hardening (a), Experimental equipment of laser surface melted hardening (b)

Fig. 2

Cross-section of laser surface melting layer

Fig. 3

Schematic illustration of lase surface melting layer

Fig. 4

Hardness distributions of width(a) and depth(b) direction in the melting zone

Fig. 5

Optical microstructures and SEM structures of laser surface melting layer (a), (d) melted zone, (b),(e) remelted zone, (c), (f) HAZ in previous melted zone

Fig. 6

Optical microstructures of laser surface melted zone

Fig. 7

Optical(a), SEM(b) microstructure and EPMA mapping results showing distribution of elements in melted zone

Fig. 8

SEM microstructure of the base metal

Fig. 9

Optical microstructure between the melted zone and the base metal

Fig. 10

(a)SEM structures from the base metal to HAZ, (b)-(e) enlarged SEM structures of area denoted as BM, H1, H2, H3 in (a)

Fig. 11

(a)SEM structures from HAZ to melted zone, (b)-(e) enlarged SEM structures of area denoted as H4, H5, M1, M2 in (a)

Table 2

Hardness near area denoted as x in (a) Fig. 10 and Fig. 11

Area BM H1 H2 H3 H4 H5 M1 M2 W.Q
Hv 180~200 280~300 350~400 450~510 570~590 590~600 590~600 650~660 580

Fig. 12

Results obtained by EBSD. (a),(b) image quality map, (c), (d) inverse pole figure map. (a), (c) HAZ, (b), (d) MZ

Fig. 13

Quasi-binary phase diagram for calculated using Thermo-Calc™ software