Advanced Search  
JWJ > Volume 36(5); 2018 > Article
Das and De: Gas Metal Arc Lap Joining of Aluminium Alloys and Steel Sheets

Abstract

A coupled experimental and theoretical investigation on joining of aluminium and galvanized sheets in lap joint geometry using an advanced pulsed current gas metal arc based process is presented. The experimental study was focussed on finding suitable processing conditions to restrict the heat input, and minimize the growth of the phase layer thickness and the formation of Fe-Al intermetallic compounds along the joint interface. The theoretical study included the development of a three-dimensional heat conduction model to compute the temperature field and thermal cycles, and estimate the final joint bead profiles and phase layer thickness as a function of processing conditions. The estimated results are tested extensively for a wide range of experimental conditions. The experimentally measured and the corresponding computed results show that the dissimilar material combinations of aluminium and galvanized steel can be joined successfully by pulsed current gas metal arc with a precise control of processing conditions and heat input.

1. Introduction

Mix-material joining of aluminium and steel sheets is a challenging task due to their different melting temperatures, varying material properties, and poor solubility in solid state1). Formation of interface layer with brittle Fe-Al intermetallic compounds (IMC) is a major problem and restricting the growth of the same by controlling the heat input has remained the primary goal1,2). The reported literatures suggest that the joint quality can be improved significantly by controlling the heat input3-5). Various methods such as laser beam and laser-arc hybrid joining2,6-14), arc based joining3-5,15-23) and friction stir welding24-26) are employed to join aluminium and steel sheets with an aim to control the heat input during joining of such dissimilar material combinations.
Sierra et al.2) reported a heat input range of 120 to 150 J mm-1 for laser beam lap joining of 1 mm thick AA6016 and 1.2 mm thick galvanized (GI) steel sheet. Shabadi et al.6) joined 1.2 mm thick AA6016 and 0.7 mm thick galvanized steel sheets using a heat input of around 45 J mm-1. A relatively wider range of heat input e.g. 105 to 165 J mm-1 was employed by Zhang et al.9) and Jia et al.10) in laser beam lap joining of aluminium alloy and hot-dip galvanized steel sheets. Windmann et al.11) joined AA6016 and aluminized steel sheets, both of 1.5 mm thickness, considering a heat input range of around 240 to 330 J mm-1. In contrast to laser beam based joining processes, several authors used advanced arc based joining processes that offered superior control of heat input to join aluminium and steel sheets. Murakami et al.15) employed heat input in the range of 170 to 255 J mm-1 in pulsed GMA lap joining of 2 mm thick pure aluminium alloy and uncoated steel sheets. Su et al.16,17) and Kang and Kim18) employed a typical heat input of around 111 J mm-1 to join AA5052 and GI steel sheets in the thickness range of 1.0 to 1.2 mm. Zhang et al.19,20) reported the suitable range of heat input of around 55 to 91 J mm-1 for joining of 1 mm thick aluminium alloy and GI sheets by cold metal transfer (CMT) process. In contrast, Cao et al.3) used a higher heat input of around 200 J mm-1 in joining of AA6061 and GI steel sheets. Das et al.5,22) used a wide heat input range from 36 to 126 J mm-1 for joining aluminium alloys to GI and galvannealed (GA) steel sheets.
The formation and growth of the interface layer and the IMCs along the joint interface depend significantly on the peak temperature and resident times during which the interface remains beyond the critical temperatures for the formation of various Fe-Al IMCs13-23). Direct monitoring of the peak temperature and thermal cycles along the joint interface is difficult in laser, arc and laser-arc hybrid joining processes. Murakami et al.15) reported the interface peak temperatures of around 1000 to 1300 K (727 to 1027 °C) in joining of aluminium alloy and steel sheets using a GMA based process. Rathod and Kutsuna13) measured the peak temperature of around 1473 K (1200 °C) in laser beam joining of 1 mm thick AA5052 and 0.5 mm thick steel sheets. Peyre et al.27) predicted the interface temperature around 1023 to 1273 K (700 to 1000 °C) in laser beam lap joining of aluminium alloy and steel sheet using a heat transfer model. In a laser-hybrid joining process, Meng et al.28) estimated the interface peak temperate to be around 1473 K (1200 °C). Qin et al.29) predicted the interface peak temperature to be around 1123 to 1373 K (850 to 1100 °C) in a GMA lap joining of aluminium alloy and steel sheets. In contrast, Das et al.23) reported the maximum peak temperature in the range of around 927 ~ 1039 K (654 ~ 766 °C) for a similar process. In summary, numerical process models for lap joining of aluminium alloy and steel sheets in particular to estimate the temperature field, thermal cycles and bead profiles are rare in open literature.
A three-dimensional heat transfer model to analyse GMA lap joining of aluminium and GI steel sheets is presented in the present work to estimate the temperature profiles, thermal cycles and peak temperature along the joint interface as function of process conditions and joint geometry. The model considers the initial joint bead profile through an analytical approach as function of wire feed rate and joining speed. The computed results are validated extensively with the corresponding experimental results for a wide range of process conditions. The estimated thermal cycles along the joint interface are further used to calculate the growth of the interface layer along the joint interface, which are also validated with the corresponding measured results.

2. Experimental Setup

AA5754 and hot-dip galvanized steel sheets, 1 mm in thickness, were joined in lap configuration using 1 mm diameter AA4043 filler wire. Table 1 depicts the chemical compositions and tensile strength of the metallic sheets and the filler wire. A microprocessor controlled GMA power source, Alpha Q551, was used to perform the experiments. The sheets were overlapped by 15 mm with the AA5754 sheet on the top as shown in Fig. 1. The welding torch was positioned along the edge of the aluminium sheet at an angle of 75º in the direction of joining speed. Pure argon (99.999%) at a flow rate of 15 l min-1 was used as a shielding gas. All the experiments were performed in direct current electrode positive (DCEP) polarity. The range of process variables, shown in Table 2, were selected based on several trial experiments so that sound joint bead profiles could be obtained for all cases within the range of selected parameters. A LEM made (LT 1005-S) current transducer along with a pc-interfaced data acquisition system (Graphtech make, model no. GL 900-4) was employed for monitoring of current and voltage transients at a simultaneous sampling rate of 100 kHz.
Table 1
Chemical composition (in wt%) of the workpiece materials and filler wire
Mg Mn Zn Fe Si Cr Cu Ti Al UTS (MPa)
AA5754 2.6-3.6 0.50 0.20 0.40 0.40 0.30 0.10 0.15 Bal. 245
AA4043 (filler wire) 0.05 0.05 0.10 0.80 4.5-6.0 - 0.30 0.20 Bal. 200
C Mn P S Si Cr Cu Ti Al UTS (MPa)
Steel 0.12 0.60 0.10 0.045 0.50 - - 0.30 - 330
Fig. 1
Schematic picture of arrangement of sheets and thermocouple locations
jwj-36-5-19f1.jpg
Table 2
Process parameters considered for preparing sample joints
Wire feed rate (wf, m min-1) Current (IAG, A) Voltage (VAG, V) Joining speed (mm s-1)
4.5 51.15 12.08~12.83 7.5,10.0
5.0 56.18
5.5 61.27
6.0 66.20 7.5
The thermal cycles were measured using K-type thermocouples located at the bottom of the steel surface along the edge of the AA5754 sheet as indicated by TC1 in Fig. 1. The joint bead dimensions were measured after polishing and etching with Keller’s reagent. The Fe-Al interface layer thickness was examined through a CamScan 3200 scanning electron microscopes (SEM). The phases along the joint interface were characterized using energy dispersive spectroscopy (EDS) and Electron Probe Micro-Analyzer (EMPA) based point analysis with an electron spot diameter of 2 μm. The joint strength was evaluated in a 50 kN universal tensile testing machine (INSTRON 3369) at a crosshead speed of 1 mm min-1.

3. Methodology

3.1 Modelling of heat source and filler wire deposition

A three-dimensional steady state heat conduction analysis was carried out to simulate lap joining of aluminium alloy and GI sheet considering the workpiece moving at a constant speed with respect to a stationary heat source. The governing equation in three-dimensional Cartesian coordinate system can be written as
(1)
δδx(kδTδx)+δδy(kδTδy)+δδz(kδTδz)+Q=ρCpδTδz
where, ρ, CP and k referred to respectively the density, specific heat and thermal conductivity; and T and v depicted temperature and joining speed, respectively. Eq. (1) considers that the workpiece moves at a constant speed, v, in the negative direction of z-coordinate. The first three terms on the left side of Eq. (1) depicted conductive heat transfer in x, y and z direction. Fig. 2 depicts the boundary conditions considered here that can be represented as
(2)
kδTδn=qs+hC(T-TA)+σε(T4-TA4)=0
where n referred to the direction normal to surface; hC, ε, σ, and TA referred to surface heat transfer co-efficient, emissivity, Stefan-Boltzmann constant and ambient temperature, respectively. The first term (Eq. 2) represented heat loss due to conduction from the surface. The second term q_s depicted applied heat flux onto the surface. The third and fourth terms referred to the convective and radiative heat losses from surface to the air.
Fig. 2
Boundary conditions applied for steady state analysis
jwj-36-5-19f2.jpg
A lumped heat transfer co-efficient was applied on the steel surfaces that were open to atmosphere as23)
(3)
hC1=2.4×103εT1.61
where hC1 was in W mm-2 K-1.61, T was in K and ε was 0.32. Another lumped expression was used for the estimation of heat loss through the backing plate using a temperature dependent convective heat transfer coefficient, hC2, as23)
(4)
hC2=hb×(T300)0.2
where hb23) was considered as 60 W mm-2 K-1.2. A constant heat transfer coefficient, hA = 10 W mm-2 K-1, was applied along the AA5754 sheet surfaces as shown in Fig. 223).
A novel methodology is proposed here to estimate the arc heat source as function of the processing conditions and filler wire deposition. Fig. 3 schematically depicts the volumetric heat source and filler wire deposition that are considered for numerical analysis. The heat input was considered as a uniform volumetric heat source as
(5)
Q˙=ηIAGVAGΠ
where IAG and VAG depicted time-averaged welding current and voltage, respectively. The value of η was considered as 0.7023). The denominator term ∏ in equation (5) was estimated as the product of arc diameter and the cross-sectional area including filler wire deposit profile and a small thickness into the metallic sheets as indicated by the cross-hatched section in Fig. 3 underneath the arc.
Fig. 3
Representation of the volumetric heat source used in the present work
jwj-36-5-19f3.jpg
The deposition from the filler wire was incorporated by addition of a discrete set of elements into the solution domain following element activation and deactivation technique in ANSYS 14.5 as shown in Fig. 3. The deactivated elements were assigned with very low value of thermal conductivity to treat them as thermally insulator. As a set of deactivated elements was activated, the thermo-physical properties of filler wire were assigned to these elements. In Fig. 3, M1 represents the deactivated elements and M2 corresponds to the activated elements depicting deposition from molten filler wire in the current step. The volumetric heat source was applied on the set of activated elements which were lying under the length of arc diameter as shown in Fig. 3. Table 3 shows the thermo-physical properties of the base metals and filler wire.
Table 3
Thermo-physical properties of base metals and filler wire
 Property AA5754/ AA4043 Steel
Density, kg m−3 2680 7290
Liquidus and solidus temperature, K 925, 880 1860, 1780
Latent heat, (J kg−1) 3.98×105 2.7×105
Thermal conductivity, W m−1 K−1 218 for T > 925 K
111.60+0.09T+1.80×10-6T2 for 300 K ≤ T ≤ 925 K
50-0.04T+2×10-5T2
Specific heat, J kg−1K−1 1252 for T > 925 K
805.383+0.394T+9.98×10-5T2 for 300 K ≤ T ≤ 925 K
402.26+0.81T-4.34×10-4T2

3.2 Estimation of filler wire deposit profile and interface layer thickness

A prior estimation of the expected bead profiles was obtained analytically as function of processing conditions and thermo-physical properties of filler alloy to accommodate the discretized geometry for the modelling purpose23). The profile of the bead was presumed as ADB as shown in Fig. 4. The lines AP and OP refer to the original unmelted boundary of the top sheet. The locations of three points, A (x2), B (x1) and C (y1), along the presumed bead profile (in Fig. 4) were estimated analytically as23)
(6)
x1d=7.688116.66685×0.87834ξ
(7)
x2d=2.071461.68914×0.84153ξ
(8)
y1d=1.762650.28662×0.73899ξ
(9)
whereξ=(η(IAGVAG)/(πr2v)ρ[CP(TL-TA)+L])×(2rb)
and d, v and r referred to the filler wire diameter, joining speed and arc radius, respectively; TL, TA and L depicted respectively the liquidus and solidus temperature and latent heat of filler material23). Equation (9) shows ξ is directly related to heat input per unit volume and inversely proportional to thickness of aluminium sheet, b23). The final bead profile was contemplated based on the numerically computed temperature field as explained in the subsequent sections.
Fig. 4
Schematic diagram of bead profiles for the joint of aluminium and GI sheets
jwj-36-5-19f4.jpg
During GMA lap joining of aluminium and GI sheets, the inter-diffusion between Fe and Al along the steel surface leads to the formation of an interface layer with several Fe-Al phases. The peak temperature and resident time during which the joint interface remains beyond a critical temperature influences the growth of the phase layer and the types of Fe-Al IMCs. The coefficient of diffusion of Fe in Al is much larger than Al in Fe at temperatures above 793 K13,23,31). Therefore, the diffusion of Fe in Al was considered as negligible below 793 K. The growth of the phase layer was estimated based on the computed thermal cycle at the joint interface using following reference23) and also checked against the corresponding experimentally measured values.

4. Results and Discussion

4.1 Measured current-voltage waveforms

Fig. 5 shows the measured current and voltage waveforms in GMA joining of aluminium to GI sheets at different wire feed rates of 4.5 and 5.0 m min-1. The short-circuiting period begins with rapid increase in welding current around 150 A and drop of voltage to a very small value of 0.1 ~ 2 V. At the end of the short-circuiting period, the current is forced to reduce to a small value by digital signal processor to shear-off the molten metal from liquid bridge at a low power resulting in reduction of spatter. A peak current pulse is applied further for a very short duration to facilitate the formation of a droplet at the tip of filler wire that is allowed to grow till it formed a liquid bridge with the steel sheet. In Fig. 5(a) and (b), the average short-circuiting current and time duration were around 67 A (±3.5) and 3.3 ms (±0.23), while the arcing current increased from 45.8 A (±3.29) to 51.75 A (±3.39) and the arcing duration reduced from 9.15 ms (±1.14) to 8.47 ms (±1.29) with the increase of wire feed rate from 4.5 to 5.0 m min-1.
Fig. 5
Measured current and voltage transients for different wire feed rates of (a) 4.5 and (b) 5 m min-1. tS and tA represent short-circuiting and arcing period
jwj-36-5-19f5.jpg

4.2 Computed and corresponding measured bead profiles

Fig. 6 shows a comparison between the experimentally measured and the corresponding computed bead profiles for different process conditions as presented in Table 2. The region encompassed between unmelted steel surface and the solidus temperature of aluminium (880 K) represents the computed bead profile. The maximum bead width of the deposit profile was measured along the AA5754 sheet surface. The computed and corresponding experimentally measured maximum bead widths in Fig. 6 (a) to (c) were as 5.7 and 6.2 mm, 6.6 and 7.1 mm, and 4.7 and 5.1 mm, respectively. The corresponding estimated heat input was as 63.30, 70.69 and 58.77 J mm-1, respectively. Likewise, the computed and corresponding measured values of the maximum bead height in Fig. 6(a) to (c) confirmed to around 1.7 ~ 1.9 mm.
Fig. 6
Comparisons of computed and corresponding measured bead profiles in joining of AA5754 to GI sheet at different wire feed rates (m min-1) and joining speeds (mm s-1): (a) (4.5, 7.5), (b) (5, 7.5) and (c) (5, 10). The compute and measured values of maximum bead width (w) and bead height (h) are (mm): (a) (5.7, 6.2) and (1.8, 1.8), (b) (6.6, 7.1) and (1.9, 1.8) and (c) (4.7, 5.1) and (1.7, 1.8). Temperature (K) values against the corresponding colour bands are shown below the figures
jwj-36-5-19f6.jpg
A comparison of Fig. 6(a) and (b) showed that increase in heat input as increase in wire feed rate from 4.5 to 5.0 m min-1 at a given joining speed of 7.5 mm s-1 increased the dimensions of bead profile that was attributed to the increase in filler wire deposition per unit length at higher wire feed rate. In contrast, Fig. 6(b) and (c) depict an increase in joining speed from 7.5 to 10.0 mm s-1 at a constant wire feed rate of 5.0 m min-1 results in a decrease in the filler wire deposition per unit length and a corresponding decrease in the bead dimensions. In general, Fig. 6(a) to (c) show a fair trend between the computed and the corresponding measured bead profiles in lap joint configuration. Fig. 6 also indicates that the molten deposit forms a fusion joint with aluminium sheet and diffusion bond with GI sheet as the maximum temperature is above the solidus temperature of aluminium and below the liquidus temperature of the steel.

4.3 Computed and corresponding measured thermal cycles

Fig. 7(a) shows computed and corresponding measured thermal cycles at thermocouple monitoring location for wire feed rate of 5.0 m min-1 and joining speed of 7.5 mm s-1 (Fig. 6b). The computed and the corresponding measured values of peak temperature were 931 K. Fig. 7(a) shows a fair proximity between the computed and the corresponding measured thermal cycles for a specific processing condition. Similar match between the computed and the corresponding experimentally measured thermal cycles are also achieved for all the other processing conditions indicated in Table 2. Fig. 7(b) further shows the location at joint interface that is considered to note the maximum peak temperature for a given process condition and, Fig. 7(c) shows the computed interface thermal cycles at the same location for two different wire feed rates of 4.5 and 5.0 m min-1 and a constant joining speed of 7.5 mm s-1. The computed peak temperature in Fig. 7(c) increased from 1061 to 965 K with an increase in wire feed rates from 4.5 to 5.0 m min-1.
Fig. 7
(a) Comparison of numerically computed and corresponding measured thermal cycles for wire feed rate of 5 m min-1 and joining speed of 7.5 mm s-1. The computed and measured peak temperatures are 931K, (b) location of computed interface thermal cycle that experiences maximum peak temperature along the interface, (c) numerically computed interface thermal cycles at constant joining speed of 7.5 mm s-1 for different wire feed rates of 4.5 and 5 m min-1
jwj-36-5-19f7.jpg

4.4 Computed interface peak temperature and corresponding resident time, and estimated and corresponding measured interface phase layer thickness

Fig. 8(a) shows the computed interface peak temperatures and calculated resident time above 793 K as function of wire feed rate and joining speed. At a constant speed of 7.5 mm s-1, an increase in wire feed rate from 4.5 to 6.0 m min-1 resulted in an increase in peak temperature and resident time from 965.3 to 1115.6 K (marked by inverted triangle) and 2 to 4.4 s (marked by straight triangle), respectively. That could be attributed to rise in heat input at higher wire feed rate. An increase in the wire feed rate from 4.5 to 5.5 m mim-1 at a highest speed of 10.0 mm s-1 led to rise in both the interface peak temperature and resident time respectively from 930.6 to 999 K (marked by hexagon) and 1.1 to 1.4 s (marked by pentagon). Fig. 8(a) illustrates that the heat input has a profound influence on the interface peak temperature and resident time. Murakami et al.15) and Qin et al.29) reported similar range of interface peak temperatures of around 1000 to 1300 K in GMA lap joining of aluminium alloy and steel sheets.
Fig. 8
(a) Computed peak temperature and resident time above 793 K along joint interface as a function of wire feed rate at two different joining speeds (v) of 7.5 and 10 mm s-1. (b) Estimated (dE) and corresponding experimentally measured (dM) phase layer thicknesses at two different joining speeds (v) of 7.5 and 10 mm s-1
jwj-36-5-19f8.jpg
Fig. 8(b) shows the comparison of analytically estimated and corresponding experimentally measured interface phase layer thickness for different joining conditions. Fig. 8(b) depicts increasing wire feed rate from 4.5 to 6.0 m min-1 at a constant speed of 7.5 mm s-1 increases the analytically estimated phase layer thickness from 1.3 to 4.8 μm (marked by circle), and the corresponding experimentally measured layer thickness varies from 2.5 (±0.29) to 6 μm (±0.37) (marked by square). At highest joining speed of 10.0 mm s-1, the estimated layer thickness increases from 1 to 2.1 μm (marked by star) as an increase in wire feed rate from 4.5 to 5.5 m min-1. The corresponding experimentally measured values of layer thickness at the joint interface were increased from 1.7 (±0.18) to 2.4 μm (±0.30) (marked by rhombus). Fig. 8(b) shows estimated interface phase layer thickness values are around 0.12 to 0.5 times lower than that of the measured phase layer thickness. The inconsistency between the estimated and the measured layer thicknesses is attributed to neglect the formation of multiple intermetallic compounds and the effect of the same on the growth of layer thickness.
In summary, the GMA lap joining of AA5754 and galvanized steel sheets was found practical with fine control of pulse current parameters to restrict the heat input. A maximum joint strength of around 207 MPa5) could be achieved for a wire feed rate of 5 m min-1 and welding speed of 10 mm s-1 that corresponded to a linear heat input of 58.77 J mm-1. It can be noted that the maximum joint strength corresponds nearly 80% of the ultimate tensile strength of the aluminum base material that is used here. A prior estimation of the adequate heat input and the resulting bead profile, thermal cycles as well as phase layer thickness along the joint interface can be obtained using an appropriately constructed numerical process model as presented in the current work. The computed and the corresponding experimentally measured results that are presented here provide a guideline to examine the suitability of this technology further for real applications in the related user applications.

5. Conclusion

A coupled experimental and numerical analysis was carried out in multi-material joining of AA5754 to hot-dip galvanized sheets, both of 1 mm thickness, by an advanced pulsed current GMA process in lap joint configuration. A novel methodology is used for a heat conduction based thermal analysis of the process that could provide reliable estimate of bead profile, thermal cycles and phase layer thicknesses as function of process conditions, joint geometry and workpiece and filler alloy properties with little simplified assumptions. The growth of the phase layer thickness along the joint interface was estimated considering the progressive solidification of the molten filler wire deposit. The overall results suggest a critical need to control the heat input during joining of aluminium and steel multi-material assembly using arc and laser beam based processes.

Acknowledgement

Authors would like to acknowledge the support of M/s EWM GmbH for providing the automotive grade aluminium alloy and hot-dip galvanized steel sheets to carry out this research work.

References

1. Agudo L, Eyidi D, Schmaranzer CH, Arenholz E, Jank N, Bruckner J, Pyzalla AR. Intermetallic FexAly-phases in a steel/Al-alloy fusion weld. Journal of Materials Science. 42 (12) (2007), 4205–4214 https://doi.org/10.1007/s10853-006-0644-0
crossref
2. Sierra G, Peyre P, Beaume FD, Stuart D, Fras G. Steel to aluminium braze welding by laser process with Al-12Si filler wire. Science and Technology of Welding and Joining. 13 (5) (2008), 430–437 https://doi.org/10.1179/174329308X341852
crossref
3. Cao R, Sun JH, Chen JH, Wang P. Cold metal transfer joining of aluminum alloys-to-galvanized mild steel. Journal of Materials Processing and Technology. 213 (10) (2013), 1753–1763 http://dx.doi.org/10.1016/j.jmatprotec.2013.04.004
crossref
4. Zhang HT, Feng JC, He P, Zhang BB, Chen JM, Wang L. The arc characteristics and metal transfer behaviour of cold metal transfer and its use in joining aluminium to zinc-coated steel. Materials Science and Engineering A. 499 (1-2) (2009), 111–113 https://doi.org/10.1016/j.msea.2007.11.124
crossref
5. Das A, Shome M, Goecke SF, De A. Joining of aluminium alloy and galvanized steel using a controlled gas metal arc process. Journal of Manufacturing Processes. 27 (2017), 179–187 https://doi.org/10.1016/j.jmapro.2017.04.006
crossref
6. Shabadi R, Suery M, Deschamps A. Characterization of joints between aluminum and galvanized steel sheets. Metallurgical and Materials Transactions A. 44A (6) (2013), 2672–2682 https://doi.org/10.1007/s11661-012-1605-7
crossref
7. Dharmendra C, Rao KP, Wilden J, Reich S. Study on laser welding-brazing of zinc coated steel to aluminum alloy with a zinc based filler. Materials Science and Engineering A. 528 (3) (2011), 1497–1503 https://doi.org/10.1016/j.msea.2010.10.050
crossref
8. Thomy C, Vollertsen F. Laser-MIG hybrid welding of aluminium to steel-effect of process parameters on joint properties. Welding in the World. 56 (5-6) (2012), 124–132 https://doi.org/10.1007/BF03321356
crossref
9. Zhang MJ, Chen GY, Zhang Y, Wu KR. Research on microstructure and mechanical properties of laser keyhole welding-brazing of automotive galvanized steel to aluminum alloy. Materials and Design. 45 (2013), 24–30 https://doi.org/10.1016/j.matdes.2012.09.023
crossref
10. Jia L, Shichun J, Yan S, Cong N, Junke C, Genzhe H. Effects of zinc on the laser welding of an aluminum alloy and galvanized steel. Journal of Materials Processing and Technology. 224 (2015), 49–59 https://doi.org/10.1016/j.jmatprotec.2015.04.017
crossref
11. Windmann M, Rottger A, Kugler H, Theisen W, Vollertsen F. Laser beam welding of aluminum to Al-base coated high-strength steel 22MnB5. Journal of Materials Processing and Technology. 217 (2015), 88–95 https://doi.org/10.1016/j.jmatprotec.2014.10.026
crossref
12. Borrisutthekul R, Yachi T, Miyashita Y, Mutoh Y. Suppression of intermetallic reaction layer formation by controlling heat flow in dissimilar joining of steel and aluminium alloy. Materials Science and Engineering A. 467 (1-2) (2007), 108–113 https://doi.org/10.1016/j.msea.2007.03.049
crossref
13. Rathod MJ, Kutsuna M. Joining of aluminum alloy 5052 and low-carbon steel by laser roll welding. Welding Journal. 83 (1) (2004), 16s–26s

14. Gao M, Chen C, Mei S, Wang L, Zeng X. Parameter optimization and mechanism of laser-arc hybrid welding of dissimilar Al alloy and stainless steel. The International Journal of Advanced Manufacturing Technology. 74 (1-4) (2014), 199–208 https://doi.org/10.1007/s00170-014-5996-z
crossref
15. Murakami T, Nakata K, Tong H, Ushio M. Dissimilar metal joining of aluminum to steel by MIG arc brazing using flux cored wire. ISIJ International. 43 (10) (2003), 1596–1602
crossref
16. Su Y, Hua X, Wu Y. Effect of input current modes on intermetallic layer and mechanical property of aluminum-steel lap joint obtained by gas metal arc welding. Materials Science and Engineering A. 578 (2013), 340–345 https://doi.org/10.1016/j.msea.2013.04.097
crossref
17. Su Y, Hua X, Wu Y. Influence in alloy elements on microstructure and mechanical property of aluminum-steel lap joint made by gas metal arc welding. Journal of Materials Processing and Technology. 214 (4) (2014), 750–755 https://doi.org/10.1016/j.jmatprotec.2013.11.022
crossref
18. Kang M, Kim C. Joining Al 5052 alloy to aluminized steel sheet using cold metal transfer process. Materials and Design. 81 (2015), 95–103 https://doi.org/10.1016/j.matdes.2015.05.035
crossref
19. Zhang HT, Feng JC, He P, Hackl H. Interfacial microstructure and mechanical properties of aluminium-zinc-coated steel joints made by a modified metal inert gas welding-brazing process. Materials Characterization. 58 (2007), 588–592 https://doi.org/10.1016/j.matchar.2006.07.008
crossref
20. Zhang HT, Feng JC, He P. Interfacial phenomena of cold metal transfer (CMT) welding of zinc coated steel and wrought aluminium. Materials Science and Technology. 24 (11) (2008), 1346–1349 https://doi.org/10.1179/174328407X213152
crossref
21. Zhang H, Liu J. Microstructure characteristics and mechanical property of aluminum alloy/stainless steel lap joints fabricated by MIG welding-brazing process. Materials Science and Engineering A. 528 (19-20) (2011), 6179–6185 https://doi.org/10.1016/j.msea.2011.04.039
crossref
22. Das A, Shome M, Das CR, Goecke SF, De A. Joining of galvannealed steel and aluminium alloy using controlled short circuiting gas metal arc welding process. Science and Technology of Welding and Joining. 20 (5) (2015), 402–408 https://doi.org/10.1179/1362171815Y.0000000032
crossref
23. Das A, Shome M, Goecke SF, De A. Numerical modelling of gas metal arc joining of aluminium alloy and galvanized steels in lap joint configuration. Science and Technology of Welding and Joining. 21 (4) (2016), 303–309 https://doi.org/10.1080/13621718.2015.1104206
crossref
24. Elrefaey A, Gouda M, Takahashi M, Ikeuchi K. Characterization of aluminum/steel lap joint by friction stir welding. Journal of Materials Engineering and Performance. 14 (1) (2005), 10–17 https://doi.org/10.1361/10599490522310
crossref
25. Kimapong K, Watanabe T. Lap joint of A5083 aluminum alloy and SS400 steel by friction stir welding. Materials Transactions. 46 (4) (2005), 835–841 https://doi.org/10.2320/matertrans.46.835
crossref
26. Chen YC, Nakata K. Effect of the surface state of steel on the microstructure and mechanical properties of dissimilar metal lap joints of aluminum and steel by friction stir welding. Metallurgical and Materials Transactions A. 39A (2008), 1985–1992 https://doi.org/10.1007/s11661-008-9523-4
crossref
27. Peyre P, Sierra G, Beaume FD, Stuart D, Fras G. Generation of aluminium-steel joints with laser-induced reactive wetting. Materials Science and Engineering A. 444 (1-2) (2007), 327–338 https://doi.org/10.1016/j.msea.2006.09.111
crossref
28. Meng X, Qin G, Su Y, Fu B, Ji Y. Numerical simulation of large spot laser +MIG arc brazing-fusion welding of Al alloy to galvanized steel. Journal of Materials Processing and Technology. 222 (2015), 307–314 https://doi.org/10.1016/j.jmatprotec.2015.03.020
crossref
29. Qin G, Su Y, Meng X, Fu B. Numerical simulation on MIG arc brazing-fusion welding of aluminum alloy to galvanized steel plate. The International Journal of Advanced Manufacturing Technology. 78 (9-12) (2015), 1917–1925 https://doi.org/10.1007/s00170-014-6529-5
crossref
30. Kobayashi S, Yakou T. Control of intermetallic compound layers at interface between steel and aluminum by diffusion-treatment. Materials Science and Engineering A. 338 (1-2) (2002), 44–53 https://doi.org/10.1016/S0921-5093(02)00053-9
crossref
31. Mehrer H. Diffusion in solid metals and alloy, Numerical data and functional relationship in science and technology. Springer Verlag, Berlin. 26 (1990), 129–152

TOOLS
PDF Links  PDF Links
PubReader  PubReader
ePub Link  ePub Link
Full text via DOI  Full text via DOI
Download Citation  Download Citation
CrossRef TDM  CrossRef TDM
  E-Mail
  Print
Share:      
METRICS
0
Crossref
1,105
View
97
Download
Related articles
Laser and Gas Metal Arc Based Dissimilar Joining of Automotive Aluminium Alloys and Steel Sheets - A Review  2018 October;36(5)
Design of Helical SPR for Joining Advanced High Strength Steel and Aluminum Alloy Sheets  2015 December;33(6)
High Current Arc Welding Technology of Aluminum Alloy  2013 February;31(1)
Laser Welding of Automotive Aluminum Alloys  2011 August;29(4)
Recent Technological Tendency of Joining for Light Aluminium Alloy  2011 June;29(3)
Laser and Gas Metal Arc Based Dissimilar Joining of Automotive Aluminium Alloys and Steel Sheets - A Review  2018 October;36(5)
Design of Helical SPR for Joining Advanced High Strength Steel and Aluminum Alloy Sheets  2015 December;33(6)
High Current Arc Welding Technology of Aluminum Alloy  2013 February;31(1)
Laser Welding of Automotive Aluminum Alloys  2011 August;29(4)
Recent Technological Tendency of Joining for Light Aluminium Alloy  2011 June;29(3)
e-sciencecentral
Register for e-submission
Register here to access the e-submission system of Journal of Welding and Joining for authors and reviewers.
Manuscript Submission
To submit a manuscript, please visit the Journal of Welding and Joining e-submission management system at http://submit.e-jwj.org, read the Instructions for Authors, and log into the Journal of Welding and Joining e-submission system. For assistance with manuscript submission, please contact: koweld@kwjs.or.kr.
Free archive
Anyone may access any past or current articles without logging in.
Editorial Office
The Korea Science and Technology Building, New B/D, Room 503
Teheran-ro 7-gil, 22(635-4, Yeoksam-Dong), Gangnam-gu, Seoul 06130, Korea
TEL : +82-2-538-6511    FAX : +82-2-538-6510   E-mail: koweld@kwjs.or.kr
Browse Articles |  Current Issue |  For Authors and Reviewers |  About