Ju, Ryu, Lim, and Cho: A Study on the Measuring Method of Work Parameters to Evaluate the Skill of FCAW Welding Trainee

Abstract

On industrial sites, FCAW is mostly performed by welders. In general, welder functional level evaluation is performed based on the appearance and mechanical testing of beads after welding. However, the actual welding quality obtained in the field is determined by the fluctuating characteristics of the working variables, depending on the welder’s skill. Therefore, with trainees, a rating system is needed to evaluate proficiency by measuring work parameters. In this study, two welding cameras were used to measure the work parameters of a welder who performed FCAW semi-automatic welding using CO2 gas. A method of grading the welder’s proficiency by analyzing the average and standard deviation of work parameters, taking into account the important factors that affect weld quality, is presented. For Trainee to develop a desire to grow on their own, a method of grading proficiency was proposed using the changing characteristics of the work variables rather than the welding results.

1. Introduction

FCAW is mostly conducted by semi-automatic welding. In Korea, FCAW welders are most active in workshops such as shipyards. The welder’s skill is typically evaluated by recording the results of defects, appearance of beads, etc. after welding, it can also be evaluated through mechanical tests. However, the welding quality obtained in the field is determined by the variation characteristics of the work parameters according to the welder’s skill. Therefore, a simple and economic evaluation system is necessary to evaluate the skill of welding trainees by measuring the work parameters1-3). Moreover, when grading the skill of trainees, it must be evaluated by more rationally measuring the operations of actual welders. By scoring the work parameters’ variation characteristics and providing feedback to the trainees, they can develop greater interest and focus on honing their skills. Accordingly, this study seeks to establish a method for measuring the work parameters of FCAW welders, quantify the variation characteristics of the work parameters, and propose a method for grading their welding skill.

2. Experimental method

2.1 Measured Four Work Parameters

The four main work parameters measured in this study are torch height, welding speed, work angle, and travel angle4-6). Torch height refers to the contact tip-to-workpiece distance (CTWD). Variations in these work parameters depend on the welder’s skill and act as a factor that directly impacts welding quality. These variations in work parameters, the welder’s empirical skill, were quantified and applied to the welder’s skill evaluation and quality control.

2.2 Specimen and experimental method

The base metal used in this study was a 150 X 100 X 6 mm SM400. Four welders performed BOP welding in the flat position on the FCAW used in welder training. Welders A and B conducted straight welding, while welders C and D conducted weaving welding. Table 1 shows the welding conditions used in the experiment.
Table 1
Welding condition of flat position FCAW
Filler metal AWS A5.20 E71T-1C 1.2mm
Base metal SM400 150 X 100 X 6 mm
Current 170~230 A
Voltage 21.6~25.4 V

2.3 Work parameter photography and measurement

Fig. 1 shows the arrangement of the welding cameras used in this experiment. A camera was arranged to photograph the side of the welding process and captured the welding speed, torch height, and travel angle (θT). Another camera was arranged to photograph the front of the welding process and captured the work angle (θW) and torch height.
Fig. 1
Arrangement of welding cameras
jwj-38-3-295gf1.jpg
Accounting for the distance between the camera and measurement target, just before welding, the side camera photographed a scale bar on a welding plate. Fig. 2 shows the photographed scale bar. To measure the torch height, travel angle (θT), and welding speed, still images were acquired at 1-second intervals from the arc starting point of images captured by the side camera. Accordingly, the still images and scale bar were used to measure the torch height, travel angle (θT), and welding speed at 1-second intervals. Fig. 3 shows the measurement of travel angle (θT), welding speed, and torch height by the side camera. Fig. 4 shows the measurement of work angle (θW) by the front camera. To correct the torch height error, it was calculated considering the work angle (θW).
Fig. 2
Scale bar on welding plate
jwj-38-3-295gf2.jpg
Fig. 3
Measurement by side camera video
jwj-38-3-295gf3.jpg
Fig. 4
Measurement by front camera video
jwj-38-3-295gf4.jpg

3. Experimental results and discussion

3.1 Measurements of work parameters

Fig. 5 shows the torch height variations when welders A and B performed straight welding. Fig. 6 shows the torch height variations when welders C and D performed weaving welding.
Fig. 5
Torch height variation graph of welder A and B
jwj-38-3-295gf5.jpg
Fig. 6
Torch height variation graph of welder C and D
jwj-38-3-295gf6.jpg
Fig. 7 shows the welding speed variations when welders A and B performed straight welding. Fig. 8 shows the welding speed variations when welders C and D performed weaving welding.
Fig. 7
Welding speed variation graph of welder A and B
jwj-38-3-295gf7.jpg
Fig. 8
Welding speed variation graph of welder C and D
jwj-38-3-295gf8.jpg
Fig. 9 shows the work angle variations when welders A and B performed straight welding. Fig. 10 shows the work angle variations when welders C and D performed weaving welding.
Fig. 9
Work angle variation graph of welder A and B
jwj-38-3-295gf9.jpg
Fig. 10
Work angle variation graph of welder C and D
jwj-38-3-295gf10.jpg
Fig. 11 shows the travel angle variations when welders A and B performed straight welding. Fig. 12 shows the travel angle variations when welders C and D performed weaving welding.
Fig. 11
Travel angle variation graph of welder A and B
jwj-38-3-295gf11.jpg
Fig. 12
Travel angle variation graph of welder C and D
jwj-38-3-295gf12.jpg
Table 2 presents the mean and standard deviation of the work parameters of welders A to D. To assess whether they were within the normal range of work parameters, the mean values of the work parameters were calculated. Moreover, since variations in the welder’s work parameters impact the welding quality, the standard deviation was calculated to evaluate the variation in work parameters4).
Table 2
Average and standard of working parameter of welder A~D
Welder Statistical method Torch height Welding speed Work angle Travel angle
A Average 26.35 33.9 3.68 34.92
Standard Dev. 1.36 1.95 0.81 0.59
B Average 18.03 39.9 0.78 7.59
Standard Dev. 2.75 2.28 0.99 0.98
C Average 26.35 33.9 3.68 34.92
Standard Dev. 1.36 1.95 0.81 0.59
D Average 18.03 39.9 0.78 7.59
Standard Dev. 2.75 2.28 0.99 0.98

3.2 Evaluation method of work parameters

To evaluate the skill of welders A-D, scores were assigned considering the mean and standard deviation of the work parameters. Weights were assigned as follows considering the importance of the work parameters impacting welding quality. The weight of torch height was assigned 3, welding speed 2, work angle 1, and travel speed 1. For torch height, the score was deducted when the mean deviated from the standard of 15 mm. For welding speed, the score was deducted as the mean decreased, and for weaving welding, a lower level range than straight welding was applied. For work angle and travel angle, the score was deducted when the mean deviated from the standard of 0°. The greater the standard deviation of the work parameter, the more the score was deducted. The mean and standard deviation were reflected in the evaluation scores with equal weight. Table 3 shows the score distribution for the mean and standard deviation. Table 4 is a classification table according to the total evaluation scores.
Table 3
Score table based on average and standard deviation of working parameters
Torch height Welding speed Work angle Travel angle Score
Straight Weaving
Average Within 15±2 Over 50 Over 30 0±2° 0±6° 5
Within 15±4 Over 40 Over 25 0±4° 0±12° 4
Within 15±6 Over 30 Over 20 0±6° 0±18° 3
Within 15±8 Over 20 Over 15 0±8° 0±24° 2
Within 15±10 Over 10 Over 10 0±10° 0±30° 1
Standard Dev. 0~1 0~1 0~1 0~1 5
1~2 1~2 1~2 1~2 4
2~3 2~3 2~3 2~3 3
3~4 3~4 3~4 3~4 2
4~5 4~5 4~5 4~5 1
Weight 3 2 1 1
Table 4
Classification table by total score
Total score
0~ 10 11~20 21~30 31~40 41~50 51~60 61~70
Grade 1 2 3 4 5 6 7

3.3 Work parameter evaluation results of welders A-D

Table 5 shows the evaluation scores for the work parameters of welders A-D. Welder 7 showed the highest score at 67, and was thus assigned Grade 7. Welders B and C scored 52 and 55 points, respectively and both were assigned Grade 6. Welder A was assigned Grade 4 with 40 points. The welders who participated in this evaluation were highly skilled in the field and thus obtained high grades. However, when beginner trainees receive a low grade, their individual welding operations are quantitatively analyzed and the welder’s skill is evaluated, thereby serving as individual feedback. Therefore, this system enables high-efficiency training and the trainee’s psychology growth, inducing them to easily concentrate.
Table 5
Score and grade of welder A ~ D
Welder Average score Standard Dev. Score Total score Grade
A 10 30 40 4
B 27 25 52 6
C 27 28 55 6
D 33 34 67 7
Fig. 13 is a graph of the four welders’ grades expressed in the form of probability density functions. As the welders were all highly skilled, they are distributed among the higher grades. Meanwhile, beginners will be distributed among the lower grades, and the distribution characteristics will differ widely according to the learning group. Since these distribution characteristics can be used to easily evaluate the level of a group or corporate organization, they can also be easily applied to welding contracts.
Fig. 13
Distribution of welder’s grade in the form of probability density function
jwj-38-3-295gf13.jpg

4. Conclusions

To evaluate the functional levels of FCAW welders using work processes rather than welding results, the variation characteristics of four main work parameters (welding speed, torch height, work angle, and travel angle) were recorded in videos, measured, and analyzed, and the following conclusions were drawn.
  • 1) This study proposed a method of measuring four main work parameters at 1-second intervals by taking videos of welders directly using an arc front camera, side camera, and scale.

  • 2) When the welders’ skill were evaluated considering the welding parameter’s importance in quality: the weight of torch height was assigned 3, welding speed 2, work angle 1, and travel angle 1.

  • 3) A system was presented in which the mean and standard deviation of the four work parameters are evaluated, scored with equal weight, and then provided to the trainees as feedback, though which they can hone their own skills.

  • 4) A method was proposed for statistically evaluating the skill of a group or corporate organization by grading the welders’ skill from 1 to 7, based on evaluation of the variation characteristics of the work parameters.

Acknowledgments

This study was supported by the KEIT research fund of the Ministry of Trade, Industry and Energy. [No: 20003633]

ORCID

ORCID: Hyeong Chang Ryu: https://orcid.org/0000-0001-5382-6795
ORCID: Kyeong Seob Lim: https://orcid.org/0000-0001-6733-0643

References

1. Wu C. S. Microcomputer-based welder training simulator. Comput Ind. 20 (3) (1992), 321–325 https://doi.org/10.1016/016613615(92)90080-7
crossref
2. Fast K, Gifford T, Yancey R. Virtual training for welding. Third IEEE and ACM International Symposium on Mixed and Augmented Reality (ISMAR 2004), Arlington, USA. (2004)
crossref
3. Hwang S. H. A study on Korean welding education and qualification system(I). J. Korean Weld. Join. Soc. 20 (2) (2002), 4–12

4. Stone R, Watts K, Zhong P, Wei C. S. Physical and cognitive effects of virtual reality integrated training. Hum Factors. 53 (5) (2011), 558–572 https://doi.org/10.1177/001∐811413389
crossref
5. Steven W, Dirk R, Mores P, Christoph B, Terrence C. Virtual reality welder training. J. Ship Prod. Des. 22 (3) (2006), 126–138 https://doi.org/10.1117/12.840473

6. Choi E, Kim J. Y, Shin S. H, Kim S. Y. A study on the analysis effectiveness of the virtual welding simulator for welding manpower development. J. Weld. Join. 33 (3) (2015), 40–46 https://doi.org/10.5781/jwj.2015.33.3.40
crossref pdf
TOOLS
PDF Links  PDF Links
PubReader  PubReader
ePub Link  ePub Link
Full text via DOI  Full text via DOI
Download Citation  Download Citation
CrossRef TDM  CrossRef TDM
  E-Mail
  Print
Share:      
METRICS
0
Crossref
400
View
16
Download
Related articles
A Study on Spatter Tracking Algorithm for a Vertical GMA Welding Process  2019 August;37(4)
A Study on the Measurement of Stress Intensity Factors for the Fatigue Crack Propagation  2012 December;30(6)
A Study on the Optimal Welding Methods of Vertical Welding Positions in the Vehicle Body  2010 December;28(6)
A Study on the Distortion of a Thin Plate Panel by Laser Welding  2007 February;25(1)
A Study on the Development of Evaluation Method for the Output Characteristics of Welding Machine by 60  2003 October;21(6)
A Study on Spatter Tracking Algorithm for a Vertical GMA Welding Process  2019 August;37(4)
A Study on the Measurement of Stress Intensity Factors for the Fatigue Crack Propagation  2012 December;30(6)
A Study on the Optimal Welding Methods of Vertical Welding Positions in the Vehicle Body  2010 December;28(6)
A Study on the Distortion of a Thin Plate Panel by Laser Welding  2007 February;25(1)
A Study on the Development of Evaluation Method for the Output Characteristics of Welding Machine by 60  2003 October;21(6)
e-sciencecentral
Register for e-submission
Register here to access the e-submission system of Journal of Welding and Joining for authors and reviewers.
Manuscript Submission
To submit a manuscript, please visit the Journal of Welding and Joining e-submission management system at http://submit.e-jwj.org, read the Instructions for Authors, and log into the Journal of Welding and Joining e-submission system. For assistance with manuscript submission, please contact: koweld@kwjs.or.kr.
Free archive
Anyone may access any past or current articles without logging in.
Editorial Office
#304, San-Jeong Building,
23, Gukhoe-daero 66-gil, Yeongdeungpo-gu, Seoul 07237, Korea
TEL : +82-2-538-6511    FAX : +82-2-538-6510   E-mail: koweld@kwjs.or.kr
Browse Articles |  Current Issue |  For Authors and Reviewers |  About
Copyright© by The Korean Welding and Joining Society. All right reserved.