Warning: fopen(/home/virtual/kwjs/journal/upload/ip_log/ip_log_2024-04.txt): failed to open stream: Permission denied in /home/virtual/lib/view_data.php on line 88 Warning: fwrite() expects parameter 1 to be resource, boolean given in /home/virtual/lib/view_data.php on line 89 Application of Plasma Arc Welding for Anti-Corrosive Material with High Molybdenum Content

Application of Plasma Arc Welding for Anti-Corrosive Material with High Molybdenum Content

Article information

J Weld Join. 2020;38(3):248-253
* WOW Metal Co., Ltd., Busan, 46744, Korea
** Division of Naval Architecture and Ocean System Engineering, Korea Maritime and Ocean University, Busan, 49112, Korea
Corresponding author : dispaul@hanmail.net
Received 2019 December 04; Revised 2020 January 13; Accepted 2020 May 25.

Abstract

Plasma arc welding (PAW) is an arc welding process similar to gas tungsten arc welding, in which an electric arc is formed between a non-consumable tungsten electrode and the workpiece. When used for cutting, the plasma gas flow is increased instead of the PAW so that the deeply penetrating plasma jet cuts through the metal, and the molten metal is continuously removed as the cutting process progresses. A plasma is a gas heated to an extremely high temperature and ionized such that it becomes electrically conductive. Although very high temperatures are applied during the PAW process, the arc flame is narrow and deep and moves at a very high speed. Thus, only a small amount of heat is transferred to the weld. A filler metal can be used, depending on the joint conditions and the required mechanical and chemical properties of the materials, particularly for thick materials or gapped joints. Two modes of the plasmawelding technique were used in actual welding fabrication: the keyhole and melt-in modes for the root run and final run, respectively.

1. Introduction

Plasma arc welding (PAW) is an arc welding process similar to gas tungsten arc welding (GTAW). The PAW process was invented by Robert M. Gage in the United States in 1953 and was patented in 1957 by Union Carbide Corporation in Buffalo, New York. Since then, many related patents have been applied and registered before the first PAW equipment was released in 1964. This welding equipment showed great advantages in precision welding processes for a wide range of materials with small to medium thicknesses. Its application started with methods and in directions to better control processes in low welding currents from the beginning of introduction in industries. Today, PAW provides excellent functional and technical performances in high quality bonding and table surface modification processes such as anticorrosive hard coating in small or precision applications including electronics, micro-packaging, and precision welding of surgical instruments. In particular, plasma spray coating process has been developed and applied to the wings and bodies of airplanes and the turbine blades of rockets for many years. As shown in Fig. 1, the precision plasma bonding process is being actively applied to the manufacturing and processing of small to medium high-grade steel pipes in petrochemical plants.

Fig. 1

Smaller pipes plasma arc welding (Source: WOW Metal Co., Ltd.)

PAW is similar to GTAW in that the arc is usually formed between a non-consumable tungsten electrode made of sintered tungsten and the material to be bonded. However, a major difference between them is that in PAW the electrode is installed inside the torch body so that the plasma arc can be separated from the sphere of influence where the shielding gas is supplied inside the nozzle. Owing to this locational design of the tungsten electrode, the plasma passes through a copper nozzle in which a fine orifice is formed that shrinks the arc and allows it to flow at a fast speed close to the speed of sound and a high temperature close to 20,000°C.

2. Materials

2.1 Chemical Composition and Physical Properties of Materials

Recently, the standards for the emission of sulfides (Sox) in exhaust gas for vessels have been greatly strengthened. According to the enforcement of new standards applied from 2020, vessels are required to use fuels with a 0.5% or lower SOx content or install a desulfurization system to reduce the SOx emissions below the standard.

To prepare for this regulation, vessels can use low sulfur oils with 0.5% or lower sulfur or use a scrubber, which is a desulfurization device (Table 1). Besides, emissions can be reduced by improving the operation efficiency of the vessel or by improving the new energy efficiency design index (EEDI) for vessels, but the amount of improvement cannot satisfy the standard.

Comparison reduction method of ship’s exhaust gas

Among the above-mentioned methods, scrubbers, which are considered to be relatively inexpensive and advantageous to manufacture and install, are often selected in the current situation.

This application case report describes the application of PAW to the fabrication and welding of a scrubber, a desulfurization device for vessels, using corrosion- and heat-resistant steel. Based on this, we aim to examine the main processes and applied technologies and to promote the development of more efficient and economical welding processes.

The material used in this welding work is 6Moly (6-6.5% Mo), which is also called a super stainless steel. Its chemical composition and physical properties are listed in Tables 2 to 5. This alloy steel has raised the pitting resistance equivalent (PRE) by chemical composition and further heightened the strength and hardness by heat treatment, and was fabricated to exhibit excellent corrosion resistance in a severe corrosive environment. In particular, 6Moly has been used in scrubbers to treat SOx from the hot emissions of vessels in a marine environment. This material is being used widely in and outside the country because it has demonstrated excellent corrosion resistance comparable to the performance of other Ni alloys and pure titanium.

Standard comparison of materials for scrubber manufacturing

Mechanical properties of materials for scrubber manufacturing

Physical properties of scrubber

3. Welding Work

3.1 Chemical Composition and Mechanical Properties of Materials

The chemical composition and mechanical properties of 6Moly used for scrubber welding in this study are outlined in Tables 3 and 5, respectively. As shown in these tables, this material has excellent tensile strength and elongation properties. Moreover, it contains a high ratio of Cr and 6% or higher Mo to withstand high-temperature corrosive environments with salinity and heat. Although this material has the disadvantage of higher price than stainless steel materials such as Super Duplex, its applications are increasing owing to excellent corrosion resistance and workability for welding. In particular, it has been widely used to manufacture scrubber devices that filter SOx by being installed in waste steam pipes through which exhaust gas emissions from ships are discharged.

Chemical composition of materials for scrubber manufacturing

3.2 Filler Wire

The filler wire used for welding basically has a similar chemical composition to that of the base metal and is characterized by increased contents of Mo considering high temperature and corrosion resistance of the welded parts. IN this welding, a material with sufficiently high contents of some components such as Mo was used considering the characteristics according to the work method.

3.3 Groove Conditions and Welding Method

For the welding groove, to attain sufficient corrosion resistance of the inner part of the scrubber shell in contact with the hot exhaust gas containing SOx, a V-shaped groove (so-called Y-type groove) with a certain size of root face was maintained and the root gap was set as an air gap condition.

A typical keyhole mode was applied to the root pass and the method supplying a filler wire was adopted. After performing the root pass of the first layer in keyhole mode, the second welding pass was finished with melt-in technique. The groove angle and root surface conditions for welding joint are shown in Fig. 2. The welding process, the completed product, and the welding bead shape are briefly shown with three photographs in Fig. 3. Fig. 4 shows photographs that captured the keyhole and melt-in mode used in the welding.

Fig. 2

Groove condition of PAW

Fig. 3

Circumferential and Longitudinal welding of a scrubber shell

Fig. 4

Keyhole/Melt-in mode capture of the actual welding

3.4 Welding Conditions

The chemical composition of the wire electrode used in welding is outlined in Table 6 and the welding conditions used are listed in Table 7.

Chemical composition of wire electrode

Welding parameters for PAW

4. Welding Result and Discussion

In this welding work using PAW, the diameter of the main body of the scrubber for ships is approximately 2,300-5,000. Thus, the space is large to allow welding either inside and outside according to the work conditions. In order to attain the sufficient corrosion resistance of the inside of the scrubber through which exhaust gas passes through as mentioned above, welding from the inside to the outside is somewhat more advantageous, but outside welding may be required depending on the type of welding device or the work environment.

When welding is performed from the outside, fine and uniform backside weld beads can be expected for the welding route, that is, the inside. Here, it can be completed with single pass in I-groove with no bevel processing or root gap for up to 10-12 mm of material thickness. However, considering the bead shape and the loss of alloys in the root part, a Y-groove was created, and a good filler wire with a better corrosion resistance performance than the base metal was melted and added to the root part, thereby improving the molten metal flor and achieving stable corrosion resistance of the root part (Fig. 4a).

Fig. 4 shows captured images of the video that was taken in keyhole and melt-in mode of the actual weld zone.

4.1 Corrosion resistance of Weld Zone

Fig. 5 shows the production test specimen collected from specimens that were welded under the same conditions as actual welding. The test was performed at the air temperature of 23.5°C and a humidity of 55.1-55.2. The temperature of the FeC13 test solution was maintained at 40°C for 24 h. No pitting was found in the ferric chloride pitting test and the amount of weight loss was represented as 0.0g/m2.

Fig. 5

Photo of corrosion test(×20)

Fig. 5 below shows a photo of the corrosion test.

4.2 Appearance Quality of Beads

The table surface and back welding beads and overall appearance were uniform and smooth because of automatic welding. Fine beads were formed to the extent that the nipples on the table surface were hard to observe. In particular, the back beads were much smaller than for TIG welding due to the absence of root gap and a narrow long arc (see Fig. 3).

Therefore, additional work such as grinding of the welding beads is not necessary, except in special cases.

4.3 Productivity of Welding

Although the scrubber is large due to its structure, it has a moderate weight and a small thickness. Hence, when working with the scrubber lying on its side, it is not easy to apply automatic welding due to deflection and vibration by self-weight. Therefore, PAW was compared with manual TIG welding, because it is used mostly for scrubber manufacturing in South Korea (see Table 3). As shown in Table 8, the total welding time of PAW for the same welding field is approximately 1/7 level of manual TIG welding, showing a significant difference in welding productivity. This is because the area of the PAW groove cross-section is small, about 1/4 of that of TIG welding (one side V, groove angle 60°, root gap 2-3 mm), which is approximately 20 mm2 and PAW has a welding speed of about 4 times faster. Since the welding time is relatively short, the amount of welding material consumption is also small, and the total shielding gas consumption is much smaller. However, the reason that the consumption of purge gas Ar has a very large difference is that a local purge device could be used due to welding characteristics as well as welding time.

Welding productivity of PAW

5. Conclusion

  • 1) PAW is easy to control because the arc length is long enough and also has an advantage in filler wire supply method.

  • 2) Stable beads could be formed with a smooth weld penetration to the back of the material to be welded even in the butt joint condition without a root gap.

  • 3) The assembly time for maintaining the root gap could be significantly shortened, and it was easier to control the welding angular deformation owing to a groove with no root gap.

  • 4) The limited thickness range for single-sided welding work could be expanded by welding keyhole mode and melt-in mode in Y-type groove when a special control of the welding root or the material thickness exceeds the single pass welding range.

  • 5) In general, an increase in cost is inevitable to establish a welding process that satisfies both quality and productivity when the precision of the object to be welded is critical. This study confirmed the importance of expanding the working and application technologies of PAW as a powerful welding process that can achieve welding productivity while reducing the cost.

ORCID

ORCID: Woo-hyeon, Choe: https://orcid.org/0000-0002-2862-4873

ORCID: Ju-yong Park: https://orcid.org/0000-0003-4571-0017

References

1. Jang S. W. IMO environmental regulation trends and count- ermeasures. Korea Shipowners'Association 2018;:1–10.
2. Zheng B, Wang Q. I, Kovacevic R. Parameters Optimization for the Generation of a Keyhole Weld Pool During the Start-up Segment in VPPAW of Aluminum Alloys, The Proceedings of the Institution of Engineers Mechanical Part B. Eng J. Manuf 2142000;:393–400.
3. American Welding Society,Welding Handbook, Vol 2:Welding Processes, 8th edition. American Welding Society (AWS) Miami, UAS 1991;
4. Lincoln Electric brochure, Special alloys. Lincoln Electric UK 2017;
5. VDM Metals brochure, VDM Alloy 59. VDM Metals Germany 2017;:1–16.
6. Choe W. H. Plasma Arc Processes. WOW Metal. Co. Ltd Busan, Korea 2018;
7. Martikainen L. Conditions for achieving high quality welds in the plasma arc keyhole welding of structural steels. J. Mater. Process. Technol 521995;:68–75.
8. Barik B. K, Sathiya P, Aravindan S. Experimental Investgations On Plasma Arc Welding Of Lean Super- martensitic Stainless Steel 5th International &26th All India Manufacturing Technology. Design and Research Conference (AIMTDR 2014) Assam, India 2014;
9. Tsuchiya K, Kishimoto K, Matsunaga T, Nakano E. Studies on Plasma Arc Welding of Plate (1st Report)- Characteristics of Arc Plasma and Bead Formation. J. Japan Weld. Soc 42(6)1973;:554–566.

Article information Continued

Fig. 1

Smaller pipes plasma arc welding (Source: WOW Metal Co., Ltd.)

Table 1

Comparison reduction method of ship’s exhaust gas

Merits Demerits Remark
Using 0.5% law sulfur oil No required Main engine modifying Fuel cost increase about 40% and cooling unit may required Uncertainty of oil supplyers, Unsettled the standard of ISO8217
Install a SOx Scrubber Available using fuel oil of 3.5% Sulfur content Required facility space(reduced cargo area), to prepare about ship waste regulation Installing cost: about US$3~7 million
LNG Fuel propulsion system Remove SOx, reducible NOx and CO2 Required fuel tank space to be increased (reduced cargo area) Renovation cost:: about US$20 million

(Source: Korea Shipowners’ Association)

Table 2

Standard comparison of materials for scrubber manufacturing

JIS G 4304/4305 ASTM A240 EN 10088-2/ 10028-7
6 Moly SUS312L UNS S31254 1.4547

Table 3

Chemical composition of materials for scrubber manufacturing

Density         [g/cm3] 8.02
Specific heat       [J/kg·K] 20°C 464
Electrical resistivity    [μΩ·cm] 89.4
Thermal conductivity   [W/m·K] 12.3
Average coefficient of thermal expansion  [10-6/°C] 20~100°C 15.3
20~200°C 15.7
20~300°C 16.1
20~400°C 16.4
Young’s modulus     [MPa] 19.7 × 104
Magnetism None
Melting range       [°C] 1360~1405

Table 4

Physical properties of scrubber

C Si Mn P S Ni Cr Mo Cu N
Specification (SUS312L) ≤0.020 ≤0.80 ≤1.00 ≤0.030 ≤0.015 17.50- 19.50 19.00-21.00 6.00-7.00 0.50-1.00 0.16-0.25
Spec’ (UNS S31254) ≤0.020 ≤0.80 ≤1.00 ≤0.030 ≤0.010 17.5- 18.5 19.5- 20.5 6.0- 6.5 0.50-1.00 0.18-0.22

Table 5

Mechanical properties of materials for scrubber manufacturing

0.2% proof stress [MPa] Tensile strength [MPa] Elongation [%] Hardness
[Hv] [HB]
Specification (SUS 312L) ≥300 ≥650 ≥35 ≤230 ≤223
Specification (UNS S31254) Sheet, strip ≥310 ≥690 ≥35 - ≤223
Plate ≥310 ≥655 ≥35 - ≤223
Example Cold-rolled sheet 1.5mmt 379 744 41 182 -
Hot-rolled sheet 8mmt 361 707 53 - 187

(*Source: Nippon Yakin Kogyo Co., Ltd.)

Fig. 2

Groove condition of PAW

Fig. 3

Circumferential and Longitudinal welding of a scrubber shell

Fig. 4

Keyhole/Melt-in mode capture of the actual welding

Table 6

Chemical composition of wire electrode

AWS ERNiCrMo-13 C Si Mn P S Ni Cr Mo Cu Fe
*A 0.01 max 0.10 max 0.5 max 0.015max 0.01 max bal. 22.0- 24.0 15.0 -16.5 0.5 max 1.5 max
B 0.01 0.03 0.2 0.003 0.003 60.0 23.0 15.6 0.01 0.4

Remark:

*

A : Al;0.1-0.4, Co;0.3% max

Table 7

Welding parameters for PAW

No. of pass Filler metal Polarity Current (A) Voltage (V) Travel speed (cpm) Interpass temp. (max) Heat input (kJ/cm)
AWS Dia. (mm)
1st(root) ERNiCrMo- 13 1.2 DCEN 250-350 28-32 38-50 100°C 8.4-17.6
2nd(final) DCEN 250-350 28-32 38-50

Fig. 5

Photo of corrosion test(×20)

Table 8

Welding productivity of PAW

GTAW(manual) PAW(auto.)
Weld length 43,400 mm
No. of pass 3 2
Travel speed 80-100 mm/min 400-450 mm
Welding time 21.7 hr 3.3 hr
Wire consumption 15.6 kg 2.2 kg
Gas consumption 345 liter 26 liter